Different Compression Ratio Affected TZM Alloy Plate Tensile Fracture

Observed 40%, 60%, 82% and 90% compression rate the TZM alloy plate tensile fracture morphology found as the compression ratio increases, the degree of densification is increase and the fracture mode change from the intergranular brittle fracture, intergranular ductile fracture, transcrystalline fracture to transgranular quasi-cleavage fracture.

The un-rollding alloy plate has a lot of voids and the fracture mode is intergranular brittle fracture. Observed the SEM picture can found each grain of alloy mostly is polyhedral shape and filled with voids. In the stretching process, these voids will become a source of cracks, causing fracture, reducing tensile strength.

When the compression rate is 40%, TZM alloy plate tensile fracture morphology is intergranular ductile fracture and cleavage fracture, in which a small number of grains have transgranular fracture phenomenon. There are some voids and small TiC particle. TiC particle showed in the grain boundary will reduce the strength of grain boundary. Further, presented crystal axis organization and voids will reduce the tensile strength of the alloy.

When the compression rate is 60%, the fracture mode is mixed fracture mode which includes quasi-cleavage fracture and transgranular ductile and brittle intergranular fracture. Besides, the dimple is clearly visible and transgranular fracture grains are increase, accompanied with quasi-cleavage fracture characteristics. In addition, the more transcrystalline fracture grains increases, indicating that the grain boundary of the alloy has been some strengthening.

When the compression rate is 80%, the fracture mode is still mixed fracture. However, transgranular fracture and quasi-cleavage fracture grains have further improved. In addition, the fibrous tissue of alloy is increase and you can clearly see some tearing ridge and shallow small dimple, which mainly occurs in plastic deformation of quasi-cleavage fracture. The alloy presented quasi-cleavage fracture has higher fracture toughness property.

When compression ratio is 90%, TZM alloy plate showing obvious quasi-cleavage fracture and transgranular fracture, most grain showing transgranular fracture. Further, since plastic deformation occurs in the grains and the cracks and voids are crushed and welded, so the welding and voids on the fracture have significantly decrease, which can enhance the strength and cohesion of the alloy, improving alloy’s mechanical properties.


Email: sales@chinatungsten.com sales@xiamentungsten.com 
Tel.: +86 592 5129696/86 592 5129595
Fax: +86 592 5129797

2016年7月17日星期日

Different Annealing Temperature Affected TZM Alloy Plate Tensile Fracture

Observed at different annealing temperatures 80% compression ratio, 2.3mm TZM alloy’s tensile fracture morphology found the influence of annealing temperature on alloy’s tensile fracture (Fig.5-9). When the annealing temperature at 850 ℃, the tensile fracture of alloy is mainly transgranular fracture and there is significant cleavage steps on the fracture. In addition, there are a lot of voids in the fracture grain boundary. Besides, these holes will form the crack source stretching process, resulting alloy breakage.

After annealing at 1000 ℃, the fracture has obvious quasi-cleavage pattern river shape and cleavage steps. And this cleavage step formed in the process of crack propagation and dislocations cross-cut. Further, in the cleavage plane have some plastic deformation tearing ridge, so the alloy before breaking through a lot of plastic deformation rather than brittle fracture.

After annealing at 1150 ℃, the alloy fracture surface is similar with 1000 ℃ annealing fracture surface mainly quasi-cleavage fracture. The alloy having quasi-cleavage fracture the fracture plastic is better.

As we knew the recrystallization temperature of TZM alloy is about 1200 ℃. When the annealing temperature is 1300 ℃, the grains of alloy is more coarse and the fracture surface is relatively flat. And the fracture mode is mainly transgranular fracture and intergranular ductile fracture, indicated the plastic property has further improved. However, observed under 1300 ℃ annealing temperature alloy’s enlarged image found there has irregular particles and pits left by tensile fracture, as well as strengthening phase precipitated. This shows that when the annealing temperature is higher than the recrystallization temperature, it will weaken the dispersed phase and will reduce the mechanical properties of the alloy.

Therefore, during the stress relief annealing, the annealing temperature should be controlled below the recrystallization temperature. When the annealing temperature is higher than recrystallization temperature, although the plastic property is been improved, however the mechanical properties of the alloy is decrease.